Method details

Method number: 2727
Download documents:

These methods are meant as a guide

All methods are generic methods. This means that the methods have been developed according to the following standard: 6 specimens of 30 mm diameter clamped in a specimen holder of 160 mm diameter (MAXCY).

Grinding

  Step  PG FG 
  Surface SiC Foil #320MD-Largo
  Abrasive Type DP-Susp. P 9 µm
  Lubricant Type WaterDP-Blue
  Speed (rpm) 300150
  Force (N) / Specimen 2030
  Holder direction >>>>
  Time (min) 01:0005:00

Polishing

  Step  P  OP
  Surface MD-MolMD-Chem
  Abrasive Type DP-Susp. P 3 µmOP-S NonDry, 0,25 µm
  Lubricant Type DP-Red
  Speed (rpm) 150150
  Force (N) / Specimen 2510
  Holder direction >>><
  Time (min) 04:0002:00

Method comments

PG Time: As needed. FG Step: Lubricant DP-Blue can be replaced by Lubricant DP-Green. OP Step: For less relief OP-S can be replaced by OP-U. For Titanium and Titanium alloys: FG Step: For cp Titanium can MD-Largo with DiaPro Allegro/Largo be replaced by MD-Plan with DiaPro Plan. P Step: This step must be removed and instead the OP step is extended, running 2 minutes at a time but to 10 min. OP Step: Mix 90 ml OP-S + 10 ml hydrogen peroxide (30%). See also Application Note on www.Struers.com : "Metallographic preparation of titanium".

This method is developed to fit a standard equipment configuration.

For advice on how to adjust the method to fit your equipment, please take a look at Preparation Parameters.

The preparation time for the plane grinding (PG) step depends very much on the condition of the samples and if they are prepared as single specimens or clamped in a specimen holder. Please check the samples after the first step and repeat it if necessary.

Method related products

Product no. Product name
40500077 Log in to see prices
40600361 Log in to see prices
40700070 Log in to see prices
40500092 Log in to see prices
40700064 Log in to see prices
40400204 Log in to see prices
40500097 Log in to see prices
40600359 Log in to see prices
40700005 Log in to see prices

Login

Password
Forgot your password?

Request access

e-Shop
e-Metalog
Digital Catalouge