Method number: 2735
Download documents:

These methods are meant as a guide

All methods are generic methods. This means that the methods have been developed according to the following standard: 6 specimens of 30 mm diameter clamped in a specimen holder of 160 mm diameter (MAXCY).

Grinding

  Step  PG FG 
  Surface MD-Piano 120MD-Allegro
  Abrasive Type DP-Susp. P 9 µm
  Lubricant Type WaterDP-Green
  Speed (rpm) 300150
  Force (N) / Specimen 3035
  Holder direction >>>>
  Time (min) 02:0005:00

Polishing

  Step  P 1 P 2 OP
  Surface MD-LargoMD-DacMD-Chem
  Abrasive Type DP-Susp. P 3 µmDP-Susp. P 3 µmOP-U NonDry, 0,04 µm
  Lubricant Type DP-GreenDP-Green
  Speed (rpm) 150150150
  Force (N) / Specimen 353015
  Holder direction >>>>><
  Time (min) 05:0005:0002:00

Method comments

PG Time: As needed. P 1 Step: This step is not always necessary.

This method is developed to fit a standard equipment configuration.

For advice on how to adjust the method to fit your equipment, please take a look at Preparation Parameters.

The preparation time for the plane grinding (PG) step depends very much on the condition of the samples and if they are prepared as single specimens or clamped in a specimen holder. Please check the samples after the first step and repeat it if necessary.

Method related products

Product no. Product name
40500097 Log in to see prices
40600361 Log in to see prices
40700023 Log in to see prices
40500071 Log in to see prices
40500092 Log in to see prices
40700066 Log in to see prices
40800125 Log in to see prices
40500065 Log in to see prices
40600359 Log in to see prices

Login

Password
Forgot your password?

Request access

e-Shop
e-Metalog
Tegramin20 EN Banner